楼主: yangmin

讨论下sio2在镀膜时冲o2的问题

 火... [复制链接]
发表于 2009-4-13 12:56:27 | 显示全部楼层
充不充对吸收和折射率基本上没太大区别,对附着性和飘移有一点影响
发表于 2009-4-14 01:57:09 | 显示全部楼层
14# guangang


O2 can make sure the film is fully oxidized.
Too much O2 cause the tooling factor changes, film packing density decreases, refractive index decreases. The adhesion might also get worse.
Not enough O2 can't fully oxidize the film, so you can't get a reliable film if the film is exposed in air for a long time.
发表于 2009-4-14 08:08:22 | 显示全部楼层
14楼的,能不能给出结论的合理解释,谢谢!!!
发表于 2009-4-15 01:07:26 | 显示全部楼层
16# tianguosky1

Too much O2 increases the chamber pressure, if your crystal is not located at the same height of the substrate, the tooling factor changes.

Too much O2 increases the voids inside the SiO2 film, let's say, you want N_SiO2=1.45, now you can get 90% SiO2, the left 10% is void, which is Air, so the final film's refractive index decreases (0.9*1.45+0.1*1=1.405).

Less O2 causes the film not fully oxidized, after a long time expose in the air, the O2 in the air may gradually oxidize the film and change the refractive index.
发表于 2009-4-19 00:21:01 | 显示全部楼层
充氧是肯定会对材料折射率有所改变的,但是对膜牢影响不大,除非充氧太多,真空度很低了。
发表于 2009-8-23 11:58:01 | 显示全部楼层
14#,16#说的非常好!太感谢了!
发表于 2009-9-2 21:35:15 | 显示全部楼层
充氧后真空室中压强减少
发表于 2011-7-13 13:09:23 | 显示全部楼层
发表于 2011-7-14 12:52:18 | 显示全部楼层
这个还真不能一概而论!
要具体到不同的镀膜条件下去。。。
发表于 2011-7-25 11:52:24 | 显示全部楼层
sio2充氧会使产品发蒙,光洁度看起来好一点
发表于 2011-7-25 12:03:49 | 显示全部楼层
氧气多了,附着力很差
发表于 2011-9-11 10:36:34 | 显示全部楼层
您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

关注公众号

相关侵权、举报、投诉及建议等,请发 E-mail:admin@discuz.vip

Powered by Discuz! X5.0 Licensed © 2001-2026 Discuz! Team.|鄂ICP备17021725号-1

在本版发帖
关注公众号
QQ客服返回顶部